Most "2.0" filament launches come with adjectives and very few numbers. SUNLU's PP 2.0 is an exception. In a technical comparison posted on its own blog, the company sets the new polypropylene against its original PP figure by figure. The table shows a material that is far tougher under impact and also weaker in straight tension. That is a real engineering trade-off, not a free upgrade, and makers should read it that way. One caveat applies to everything below: every number comes from SUNLU and none has been independently tested.

SUNLU showed PP 2.0 at Formnext 2026 in Frankfurt (Hall 12.0, Booth C11, November 17-20), alongside a "2.0" filament range that includes PLA+ 2.0, PETG 2.0, Silk PLA+ 2.0 and High Speed PLA+ 2.0. The booth also carried the FilaDC i10 storage cabinet, a range of FilaDryers and new PC-Like and PA-Like resins. This piece is about the materials data, and polypropylene in particular, since that is where SUNLU has published the most detail.

The Numbers, Side by Side

These are SUNLU's published figures for original PP and PP 2.0:

  • Notched Izod impact: 5.3 ±1.5 vs 23 ±5 kJ/m² (about 4.3x higher)
  • Tensile strength: 19 ±3 vs 15 ±3 MPa (about 21% lower)
  • Flexural strength: 19 ±3 vs 18 ±3 MPa
  • Elongation at break: 850 ±150% vs 900 ±300%
  • Heat deflection temperature: 58.5 ±3 vs 65 ±10 °C
  • Melt flow rate: 9.75 ±2 vs 4.4 ±1 g/10 min
  • Molding shrinkage: 1.50% vs 1.36%
  • Density: 0.90 vs 1.01 g/cm³ (about 12% heavier)
  • Hardness: Shore 54.5D vs 60D

The headline figure is impact strength. A notched Izod test measures how much energy a specimen absorbs when a pendulum strikes it at a pre-cut notch. It is a reasonable proxy for how a part behaves when it is dropped, snapped shut or hit at a stress concentration. Going from about 5 to about 23 kJ/m² is a big change. Even at the bottom of PP 2.0's stated tolerance band (18 kJ/m²), the result sits well above the top of the original's band (6.8 kJ/m²).

Tensile strength moves the opposite way. The two tensile ranges overlap at their edges (16-22 MPa for the original, 12-18 MPa for PP 2.0), but the nominal values point to a weaker material under a steady pull. Flexural strength is essentially unchanged, and elongation rises slightly to 900%. Both PPs are very stretchy materials, which is a large part of why polypropylene suits living hinges at all.

Reading Between the Rows

Several of the secondary figures say more about how the material prints than about the finished part.

Melt flow rate drops by more than half. An MFR of 4.4 g/10 min against 9.75 means PP 2.0 flows less freely when molten. SUNLU does not say what that does to printing, but a stiffer melt can behave differently in the nozzle, so speed profiles tuned for the old spool may need to be revisited rather than copied across.

Shrinkage drops. SUNLU attributes polypropylene's warping and bed lifting to uneven shrinkage as the semi-crystalline plastic cools, plus poor first-layer adhesion from its low surface energy. SUNLU's figure falls from 1.50% to 1.36%. That is a modest reduction, roughly a tenth, and it supports the company's claim of better "print stability." It does not remove the adhesion problem, and SUNLU still recommends PP-specific glue or adhesive, a slow first layer and a brim for sharp or wide parts.

Heat deflection rises. At 65 °C against 58.5 °C, PP 2.0 nominally holds its shape under load at higher temperatures. The stated tolerances are wide (±10 °C for PP 2.0, ±3 °C for the original), so the two ranges overlap and the real-world gain is uncertain. For something like a housing near a warm electronics board, a margin of this kind could be useful if it holds up.

Advertisement

It is heavier and harder. Density climbs from 0.90 to 1.01 g/cm³. One of polypropylene's selling points has always been that it is among the lightest common plastics, and PP 2.0 gives some of that up. A 1 kg spool of the new material will yield less part volume than a 1 kg spool of the old one. The Shore hardness moves from 54.5D to 60D.

What It Means for Makers

SUNLU's own advice is unusually direct. Choose the original PP when light weight and tensile load matter. Choose PP 2.0 when impact resistance and print stability matter. That lines up with the data, and it maps onto real projects fairly cleanly.

PP 2.0 makes sense for the parts SUNLU itself names: clips, latches, protective housings and workshop fixtures. These are parts that get dropped, snapped or hit by sudden loads. A higher notched Izod figure is aimed at exactly that kind of event. SUNLU says the original PP also suits living hinges exposed to repeated bending, so do not assume PP 2.0 is the automatic choice there.

Advertisement

The original PP still wins for parts that carry a steady pulling load, and for anything where every gram counts. SUNLU notes the original suits lightweight housings and parts that need to float, and says PP 2.0 is less suited to drones, RC aircraft and wearables, so the 12% density penalty is a real cost there.

Plan for retuning either way. A lower melt flow rate and different shrinkage mean an old PP profile is a starting point, not a finished answer. SUNLU suggests 240-260 °C nozzle, 40 °C bed and 30-170 mm/s as a starting point. Print a test clip and a tensile coupon before committing a large job.

Drying and Storage

The other half of SUNLU's Formnext story was moisture. The company showed seven dryers: the FilaDryer S1 Plus, S2, SP2, E2, S4, S4 Pro and an AMS Heater. Alongside them was the FilaDC i10 cabinet, which SUNLU says keeps filament dry with a circulating molecular-sieve system rather than heat. 3D Printing Industry's coverage frames the split simply: the i10 keeps dry filament dry, and the S4 Pro removes moisture that a spool has already absorbed.

That division of labor is the sensible way to think about it. A storage cabinet is not a substitute for drying a wet spool, and a dryer is not a long-term home. For the rest of the 2.0 line, SUNLU claims low moisture absorption and improved interlayer bonding for PETG 2.0, and offers Silk PLA+ 2.0 in 16 shades. As with PP 2.0, those are manufacturer claims.

The hardware is currently part of a SUNLU Black Friday campaign that runs through November 30. 3D Printing Industry's piece is promotional in tone, but it makes a fair point: whether a dedicated cabinet and dryer pay for themselves depends on how much you print.

Bottom Line

PP 2.0 is not simply "better PP." By SUNLU's own numbers it is a tougher, more stable, slightly more heat-tolerant polypropylene that is weaker in tension and heavier per part. That is a good trade for snap-fits and hinges and a poor one for lightweight or tension-loaded parts. It is also refreshing to see a filament maker publish the downsides alongside the gains. Until independent tests confirm the figures, treat them as a well-documented starting point.

Sources